· Mysa

Forging Medieval Points

Machine translation. This page was machine-translated from Czech. The Czech version is authoritative.
Switch to original Czech version. · Zobrazit originál článku v češtině

Forged points belong with traditional bows just as much as feather fletchings or bone nocks on arrows. That is why, at the recent Archers' Meeting in Vsetice, the blacksmith Michal Sodja (Mýša) demonstrated in one of the workshops how to make bodkins – forged pyramid-shaped points with a socket. For those interested, he has also written this guide on how to make bodkins at home.
hrot-aed2ca.jpg

Before starting any work, it is necessary to decide what goal I am pursuing: making an imitation of a medieval point, a historical reconstruction, occupational therapy, and so on. Further, what target I will be shooting at and from what distance, and whether I am willing to risk destroying the arrow or the target butt. In other words, how much work I am willing to invest, how important it is to me to preserve historical methods, what weight the point may have, how hard a material it will penetrate, its resistance on penetration, the size of the hole the arrow will make, and whether it can be pulled out so the arrow can be used again.

Before we get to the work itself, we will need to say something about the materials used by medieval smiths, the minimum tool equipment, the possible targets of medieval points, their types and uses, and perhaps Mamutík will manage to insert the clip he filmed at my place. (Don't worry, he will. Editor's note)

Throughout the Middle Ages, and not only in Europe, the material used for all armourers' and blacksmiths' work was considerably different from anything that can be bought today. It differed in production technology, structure and mechanical properties. And it was also more expensive. You may remember from chemistry lessons how iron is produced. How steel is made probably fewer people know, and only a few initiates know what happens in steel at high temperatures and when alloying it with various elements.

Put simply, steel is an alloy of iron with carbon and other elements. Iron is soft and malleable. If its crystal lattice is disrupted by atoms of other elements, its mechanical properties change fundamentally. We will be interested mainly in hardening and tempering, that is, heating to a precise temperature and cooling. Hardening makes steel harder, but it becomes brittle. That is why it is heated again to a lower temperature and quenched again. The hardness drops somewhat, but the steel becomes tough. Iron cannot be hardened, and at a carbon content above 2% steel becomes cast iron, which is not suitable for blacksmithing.

Throughout the Middle Ages and most of the early modern period, humankind knew only one way of making steel and iron – low-temperature smelting of poor-quality ores. The Industrial Revolution brought two methods of producing iron and steel on a large scale from cast iron: puddling and finery forging. The resulting material is very similar in structure to medieval raw materials, but it contains a considerable percentage of sulphur and phosphorus and is not very suitable for blacksmithing. It cracks and tears. With the discovery of refining in induction furnaces, quality materials appeared again, which in many respects lag behind the medieval ones, while in others they are incomparably better.

So what did the medieval smith reach for? He essentially had two starting materials: poor-quality ores such as haematite, ferruginous sands and so on, and meteoritic iron. The latter, however, is found in Europe almost exclusively in Scandinavia, or it was imported. It is an alloy of iron and nickel.

Bog ores first had to be roasted, and then smelting took place in a low clay furnace. It was filled with charcoal, and once it was lit, ore and more charcoal were added. After several days of constant blowing and feeding, the lower part of the furnace was broken open and a lump of iron was taken out. Later the air supply was no longer at the lowest part of the furnace, so the result of smelting was partly steel. This lump was processed further by repeated folding and forging, so-called pile welding. This produced a homogeneous material with a layered structure, similar to wood.

If it was to become steel, it had to be enriched with carbon. Again there were two possibilities. Either a bar of iron was wrapped in a material containing organic carbon, sealed in a protective casing and kept at a high temperature for several days, or the material was carburised continuously during forging. A common way to achieve this was to wrap the pile in straw ash and pour thin clay slurry over it. The clay acted as a flux and at the same time prevented access of air.

I found such a procedure, for example, in the Kalevala, where the smith Ilmarinen makes steel from bog ore and carburises it continuously with the help of straw. The smith Wieland probably also enriched it with nitrogen. The Japanese still use it in making traditional swords. The result is steel in which high-carbon and low-carbon layers alternate regularly, with inimitable mechanical properties. Such a material was, however, correspondingly costly, and the arrow would have become quite expensive. After all, as long as it did not have to pierce armour, it was quite pointless. It was much more usual, especially in mass production, to use cheaper iron and weld a small piece of steel onto the very tip of the point, or to case-harden (surface enrichment with carbon) the finished product. It must also be borne in mind that such highly specialised craftsmen were found only in larger conurbations, whereas a village smith reached for what he had at home (nails, old tools and the like). Professionals, such as plate armourers, axe makers, arrowsmiths, swordsmiths and so on, mostly had a choice.

Assuming we are not going to be quite so pedantic and a purely visual imitation is enough for us, minimal equipment will suffice, which can be adapted for our comfort with the help of any locksmith. Unless, of course, you already have the necessary equipment at home.

First of all, we will need a sufficient source of air. For such a small object as an arrow point, one could, purely in theory, do without it, but heating would take needlessly long. For blacksmith's forges, fans or blowers providing at least 0.05 m3/s are recommended.

We will need considerably less. Hand blowers are mostly very simple in construction and almost anyone can make one. They work either on the piston principle or with bellows. In any case, they should be double-acting, that is, supplying a continuous, one-directional stream of air. In the European tradition bellows are usual, the Japanese use a box-shaped piston, in Indonesia two large bamboo pumps, and the Indians, for instance, a plastic bag. For our needs, a larger double-acting camping pump might even be sufficient, or, if there is a source of electricity, an old vacuum cleaner with power regulation and a reverse-flow option.

m-mech-35d62b.jpg

An obvious necessity is the tuyère (the part of the nozzle that will be in direct contact with the fire), made of an absolutely non-flammable material, preferably a durable one. Ideal is a thicker cast-iron pipe, heat-resistant ceramic or fireclay; in the last resort even iron, bearing in mind that we will have to replace it often and slag sticks to it easily.

Forges (fire pits) are of two types: with the air supply from below, or from the side. If you have a modern cast-iron forge, it has an air supply from below. For everyone else, a much more primitive side-blown hearth will be more convenient. It is essentially a hollow into which air is blown from the side. For greater comfort, lower fuel consumption and concentration of heat, it is good to equip it with side walls as well. For such a small object as a point, two bricks (preferably fireclay) will do. Also, if the blower is too close to the hearth, a heat-resistant screen. The size of the hollow is about 20x20 cm.

The anvil. An anvil also has its anatomy. Industrially made anvils have a whole range of features that make the smith's work easier. The most commonly seen is the Styrian anvil. It has a conical and a wedge-shaped horn for bending, a side face (a sloping surface on the side) and a square hole for fixing attachments. More rarely you will come across the English anvil (without horns), the French one (cone, pyramid, sometimes a "balcony", an upsetting heel, punching holes …) or the bickern (a tall anvil with narrow horns).

We should be interested in weight. The anvil should be heavy enough not to dance under the hammer and must be adequately secured. If you will be working away from home or a country cottage, it must be transportable. I also do not recommend leaving it permanently outside the cottage – it quickly ends up at the scrap yard.
Price difference: a new 100 kg anvil about 9,000 CZK, at the scrap yard 700 CZK!!!

When forging a point you will mostly be using light hammers and small pieces of material, so even a 30 kg locksmith's anvil, or possibly a piece of rail, will do. Outside Europe, an anvil in the shape of a large nail driven into the ground is often used. It is simple and effective enough. In the last resort a suitable stone can be used as well.

The more primitive the equipment, the greater the demands on dexterity. That is why it is good to also have supplementary tools to fit into the hole in the anvil, so-called swages.

First, a hardy – a chisel to fit into the anvil for cutting off material – then a bottom rounding swage (a groove about 2 cm in diameter) and a mandrel for straightening the socket.

m-utinka-e65806.jpg

If you do not have an anvil with a hole, everything can be attached to a block, made on a rail, or you can have a smith, locksmith or toolmaker make something for a few coins to be driven into the ground. Gradually you will also find out the suitable shape of the tools and be able to make them yourself.
Tongs for handling the point. Ideal is something like larger pliers for bending wire. These can be bought. They are the kind with two cones. The longer the handles, the greater the grip and the less you have to put your hand into the fire. Even the strongest glove heats through. Proper blacksmith's tongs for the fire can also be bought and cost from 600 CZK upwards, or you can make them yourself. You will manage fairly quickly on your own – it is a basic blacksmithing skill. Unless it is necessary, do not leave the tongs in the fire and do not put them into water if they are red!!!!! They become brittle.

The forging of the points itself is quite simple, especially in the case of armour-piercing points, so-called bodkins. They have a pyramid-shaped point and several types according to the taper of the sides. In general, one starts by making the socket – a little cone into which we then insert the arrow shaft.

It is useful to first draw the pattern of the cone on the anvil, or, for the more skilled, to make a drawing-out tool with edges identical to the edge of the cone – this will come in especially handy for other types of points, for example for a crossbow. It will essentially be an isosceles triangle with its apex on the axis of the point and an opposite side of length 3.14 x d, where d = the diameter of the shaft, with a slightly convex surface.

m-babka-ac4a64.jpg

Another important aid is the mandrel. You make it from some tougher round bar of about 10 – 12 mm diameter, on which you draw out a cone with a taper of roughly 3 : 1. Like a sharply sharpened pencil.
A suitable blank for a shaft of 8 - 9 mm diameter is a 6 x 6 mm square bar of steel with a carbon content of 0.5 - 0.7%, or in the last resort iron.

Procedure:

  • Carefully heat the material to an orange to yellow colour.
  • With the peen of the hammer (the opposite of the face), draw out a fan at the end, slightly wider than the circumference of the arrow shaft and as long as the socket is to be.m-kladivo-9108b9.jpg
  • Carefully roll it into a little cone, working from the tip outwards. Take care that the edges overlap!!!
  • Straighten the socket with the help of the mandrel and cut it off on the hardy about 1 cm before the end of the socket. m-stocittulej-abaf87.jpg m-srovnatnatrnu-7f59a8.jpg m-odseknout-8d7ed1.jpg
  • Grip the socket in the tongs and draw out the point with oblique blows. It is essential that the temperature does not drop below dark red, otherwise the material will tear. When heating, blow little or not at all and heat very carefully. The wall of the socket should be very thin and it is easy to burn it. If that happens, throw it away and start again. m-trn-91bec6.jpg
  • Heat the finished bodkin to 750-800 °C (cherry red) and immerse it in water almost up to the start of the socket.
  • After removal, the point will be heated again from the still-hot socket and the hardened, bright point will change colour. As soon as blue begins to appear, immediately immerse it again. Do not let the blue run all the way to the tip!!!

Other types of points are considerably more complicated and require a number of skills, for example an elementary knowledge of forge welding, and are not entirely suitable for beginners.

Best of luck

Gallery: Gallery with photos taken in Mýša's forge

← Content in English